Description: Plastic Clay - Allier, France
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.30% | 0.02 | |
| K2O | 1.80% | 0.07 | |
| MgO | 0.40% | 0.03 | |
| Na2O | 0.10% | 0.01 | |
| TiO2 | 1.40% | 0.06 | |
| Al2O3 | 29.50% | 1.00 | |
| SiO2 | 53.60% | 3.08 | |
| Fe2O3 | 3.30% | 0.07 | |
| LOI | 9.60% | n/a | |
| C | 0.20% | n/a | |
| Oxide Weight | 312.57 | ||
| Formula Weight | 346.53 | ||
Raw Color - Light Cream - Cream
Particle Size (e.s.d.)
125 microns - 0.3
63 microns - 1.0
20 microns - 98
2 microns - 77
.5 microns - 44
Modulus of Rupture at 110C
Mn/M2 - 4.3
lbf/in2 - 630
Water Absorption
1120C - 6.0
1220C - 0.50
Shrinkage Dry to Fired
1120C - 7.5
1220C - 8.1
Refractoriness
Cone - , 1710C
Plastic Index - 1004
PF NO. - 44.8
| Typecodes |
Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically. |
| Dry M.O.R. (50% Silica) | 665C |
|---|