SKD Ball Clay

Description: Devon Standard Ball Clay

Oxide Analysis Formula Tolerance
CaO 0.20% 0.01
K2O 1.60% 0.05
MgO 0.30% 0.02
Na2O 0.20% 0.01
TiO2 1.00% 0.04
Al2O3 32.90% 1.00
SiO2 50.00% 2.58
Fe2O3 1.20% 0.02
LOI 12.60%n/a
C 1.60%n/a
Oxide Weight 270.97
Formula Weight 315.81

Notes

Particle Size (e.s.d.)
125 microns - 0.50
10 microns - 98
2 microns - 85
1 microns - 75
Modulus of Rupture at 110C
Mn/M2 - 5.9
lbf/in2 - 850
Defloculant Required - (3:1 Na2SiO3(C.100):Na2CO3) - 0.4
Water Absorption
1120C - 7.0
1220C - 0.40
Shrinkage Dry to Fired
1120C - 14.50
1220C - 17.00
Reflectance 464nm
1120C - 77
1220C - 71
Refractoriness
Cone - 33, 1730C

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy