Description: Lead Sesquisilicate Frit
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| PbO | 68.43% | 1.00 | |
| Al2O3 | 3.06% | 0.10 | |
| SiO2 | 28.51% | 1.55 | |
| Oxide Weight | 326.17 | ||
| Formula Weight | 326.17 | ||
| Materials |
Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot. |
| Typecodes |
Leaded Frit
Frits can contain 1% or 80% PbO so this category can be misleading, check the chemistry to find out. |
| Typecodes |
Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types. |
| Frit Melting Range (C) | 880-1080 |
|---|