Alternate Names: Frit Pb1325
Description: High lead borosilicate with small amount of sodium
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| Na2O | 2.90% | 0.20 | |
| PbO | 40.80% | 0.80 | |
| B2O3 | 35.70% | 2.23 | |
| SiO2 | 20.60% | 1.49 | |
| Oxide Weight | 435.60 | ||
| Formula Weight | 435.60 | ||
| Materials |
Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot. |
| Typecodes |
Leaded Frit
Frits can contain 1% or 80% PbO so this category can be misleading, check the chemistry to find out. |
| Typecodes |
Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types. |
| Co-efficient of Linear Expansion | 7.3 x 10-6 (50-450C) |
|---|---|
| Frit Softening Point | 1260F |
| Frit Melting Range (C) | 1260-1330F |
| I.F.P. (celsius) | 490C |