Oct 22, 2026: We are working on protecting our servers against the PHP2Shell vulnerability just discovered. The CDN download server is back online. The digitalfire and insight-live servers were patched on Oct 21.
Description: Reimbold & Strick stoneware frit
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| B2O3 | 13.00% | 0.60 | |
| Na2O | 2.00% | 0.10 | |
| Al2O3 | 6.00% | 0.19 | |
| CaO | 7.00% | 0.40 | |
| PbO | 34.00% | 0.49 | |
| SiO2 | 38.00% | 2.04 | |
| Oxide Weight | 323.24 | ||
| Formula Weight | 323.24 | ||
| Materials |
Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot. |
| Typecodes |
Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types. |
| Co-efficient of Linear Expansion | 66 x 10-7 (20-400C) |
|---|---|
| Frit Softening Point | 610C |
| Glass Transition Temperature | 560C |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk