CC China Clay

Description: Devon China Clay

Oxide Analysis Formula Tolerance
CaO 0.10% -
K2O 2.40% 0.07
MgO 0.20% 0.01
Na2O 0.10% -
TiO2 0.20% 0.01
Al2O3 37.30% 1.00
SiO2 47.00% 2.14
Fe2O3 0.80% 0.01
LOI 12.00%n/a
Oxide Weight 240.92
Formula Weight 273.77

Notes

Particle Size (e.s.d.)
125 microns - <0.03
10 microns - 96
2 microns - 51
1 microns - 35
Modulus of Rupture at 110C
Mn/M2 - 1.0
lbf/in2 - 140
Defloculant Required - (3:1 Na2SiO3(C.100):Na2CO3) - 0.0
Water Absorption
1120C - 20.5
1220C - 7.00
Shrinkage Dry to Fired
1120C - 9.50
1220C - 18.50
Reflectance 464nm
1120C - 86
1220C - 84
Refractoriness
Cone - 33, 1730C

Related Information

Links

Materials Kaolin
The purest of all clays in nature. Kaolins are used in porcelains and stonewares to impart whiteness, in glazes to supply Al2O3 and to suspend slurries.
Typecodes Kaolin
Pure clay mineral, there are many brand names of varying purity and iron content.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy