Pemco Frit P-1N72

Alternate Names: 1N-72,1N72

Description: Alkali-alumina-borosilicate body frit

Oxide Analysis Formula Tolerance
K2O 1.80% 0.07
Na2O 15.80% 0.93
B2O3 24.00% 1.26
Al2O3 3.90% 0.14
SiO2 54.50% 3.31
Oxide Weight 365.03
Formula Weight 365.03

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Fusion Frit F-74
Materials Hommel Frit 4GF153A
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 9.30
Co-efficient of Linear Expansion 9.30 (50-450C)
Frit Softening Point 1400F
Frit Melting Range (C) 1350-1450F
Co-efficient of Linear Expansion 9.3x10-6 (50-450C)
I.F.P. (celsius) 587C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy