General Frit GF-18

Alternate Names: Frit 18, Frit GF18

Description: Leaded calcium frit for cone 01-5 dinnerware glazes

Oxide Analysis Formula Tolerance
CaO 10.46% 0.57
K2O 2.73% 0.09
Na2O 1.99% 0.10
PbO 17.22% 0.24
B2O3 7.83% 0.35
Al2O3 6.23% 0.19
SiO2 53.53% 2.74
Oxide Weight 307.92
Formula Weight 307.92

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Ferro Frit 3565
Materials Pemco Frit Pb-349
Materials Fusion Frit FL-4
Materials Ferro Frit 3509
Materials Hommel Frit 468
Typecodes Leaded Frit
Frits can contain 1% or 80% PbO so this category can be misleading, check the chemistry to find out.
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 6.30
Frit Softening Point 1950F

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy