May 2026: We are continuing a major code rewrite. Please contact us if you find issues. Thank you.

1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Ferro Frit 3419

Alternate Names: F3419

Description: Lead borosilicate glaze frit cone 08-02

Oxide Analysis Formula Tolerance
Na2O 6.40% 0.28
PbO 59.20% 0.72
B2O3 14.50% 0.57
SiO2 19.90% 0.90
Oxide Weight 271.40
Formula Weight 271.40

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Frit G-23
Materials Pemco Frit Pb-83
Materials Hommel Frit 33
Materials General Frit GF-42
Typecodes Leaded Frit
Frits can contain 1% or 80% PbO so this category can be misleading, check the chemistry to find out.
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 8.2 x 10-6
Frit Melting Range (C) 1400F

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy