Description: Devon China Clay
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.10% | - | |
| K2O | 2.40% | 0.07 | |
| MgO | 0.20% | 0.01 | |
| Na2O | 0.10% | - | |
| TiO2 | 0.20% | 0.01 | |
| Al2O3 | 37.30% | 1.00 | |
| SiO2 | 47.00% | 2.14 | |
| Fe2O3 | 0.80% | 0.01 | |
| LOI | 12.00% | n/a | |
| Oxide Weight | 240.92 | ||
| Formula Weight | 273.77 | ||
Particle Size (e.s.d.)
125 microns - <0.03
10 microns - 96
2 microns - 51
1 microns - 35
Modulus of Rupture at 110C
Mn/M2 - 1.0
lbf/in2 - 140
Defloculant Required - (3:1 Na2SiO3(C.100):Na2CO3) - 0.0
Water Absorption
1120C - 20.5
1220C - 7.00
Shrinkage Dry to Fired
1120C - 9.50
1220C - 18.50
Reflectance 464nm
1120C - 86
1220C - 84
Refractoriness
Cone - 33, 1730C
| Materials |
Kaolin
The purest of all clays in nature. Kaolins are used in porcelains and stonewares to impart whiteness, in glazes to supply Al2O3 and to suspend slurries. |
| Typecodes |
Kaolin
Pure clay mineral, there are many brand names of varying purity and iron content. |