Description: WBB Devon Ball Clay Group 1
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.20% | 0.01 | |
| K2O | 1.00% | 0.03 | |
| MgO | 0.20% | 0.01 | |
| Na2O | 0.10% | - | |
| TiO2 | 0.90% | 0.03 | |
| Al2O3 | 35.00% | 1.00 | |
| SiO2 | 46.20% | 2.24 | |
| Fe2O3 | 1.30% | 0.02 | |
| LOI | 13.10% | n/a | |
| C | 2.40% | n/a | |
| Oxide Weight | 247.42 | ||
| Formula Weight | 292.81 | ||
Particle Size (e.s.d.)
125 microns - 0.30
10 microns - 97
2 microns - 86
1 microns - 78
Modulus of Rupture at 110C
Mn/M2 - 4.9
lbf/in2 - 710
Defloculant Required - (3:1 Na2SiO3(C.100):Na2CO3) - 0.1
Water Absorption
1120C - 9.5
1220C - 2.50
Shrinkage Dry to Fired
1120C - 14.00
1220C - 16.50
Reflectance 464nm
1120C - 80
1220C - 76
Refractoriness
Cone - 33, 1730C
| Typecodes |
Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites. |