Description: WBB Devon Ball Clay Group 2
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.20% | 0.01 | |
| K2O | 1.40% | 0.04 | |
| MgO | 0.40% | 0.03 | |
| Na2O | 0.10% | - | |
| TiO2 | 0.80% | 0.03 | |
| Al2O3 | 33.80% | 1.00 | |
| SiO2 | 47.60% | 2.39 | |
| Fe2O3 | 1.20% | 0.02 | |
| LOI | 14.50% | n/a | |
| C | 3.00% | n/a | |
| Oxide Weight | 258.02 | ||
| Formula Weight | 312.75 | ||
Particle Size (e.s.d.)
125 microns - 1.00
10 microns - 97
2 microns - 84
1 microns - 75
Modulus of Rupture at 110C
Mn/M2 - 4.8
lbf/in2 - 700
Defloculant Required - (3:1 Na2SiO3(C.100):Na2CO3) - 0.5
Water Absorption
1120C - 9.0
1220C - 1.50
Shrinkage Dry to Fired
1120C - 14.50
1220C - 18.00
Reflectance 464nm
1120C - 80
1220C - 73
Refractoriness
Cone - 33, 1730C
| Typecodes |
Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites. |