Mae Vit W Ball Clay

Description: Thailand Ball Clay

Oxide Analysis Formula Tolerance
CaO 0.40% 0.03
K2O 2.50% 0.10
MgO 0.50% 0.05
Na2O 0.30% 0.02
TiO2 0.40% 0.02
Al2O3 27.40% 1.00
SiO2 54.30% 3.36
Fe2O3 1.40% 0.03
LOI 13.00%n/a
C 3.50%n/a
Oxide Weight 324.61
Formula Weight 388.76

Notes

Particle Size (e.s.d.)
125 microns - 3.0
20 microns - 96
2 microns - 83
.5 microns - 49
Modulus of Rupture at 110C
Mn/M2 - 6.4
lbf/in2 - 920
Water Absorption
1120C - 3.0
1220C - 0.0
Shrinkage Dry to Fired
1120C - 9.0
1220C - 11.5
Reflectance 464nm
1120C - 66
1220C - 48
Refractoriness
Cone - 32, 1710C

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.