Oct 22, 2026: We are working on protecting our servers against the PHP2Shell vulnerability just discovered. The CDN download server is back online. The digitalfire and insight-live servers were patched on Oct 21.
Description: WBB Devon Ball Clay Group 1
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.10% | 0.01 | |
| K2O | 1.80% | 0.06 | |
| MgO | 0.30% | 0.02 | |
| Na2O | 0.20% | 0.01 | |
| TiO2 | 0.90% | 0.03 | |
| Al2O3 | 33.90% | 1.00 | |
| SiO2 | 49.40% | 2.47 | |
| Fe2O3 | 1.00% | 0.02 | |
| LOI | 12.40% | n/a | |
| C | 1.80% | n/a | |
| Oxide Weight | 263.58 | ||
| Formula Weight | 307.20 | ||
Particle Size (e.s.d.)
125 microns - 0.40
10 microns - 98
2 microns - 84
1 microns - 74
Modulus of Rupture at 110C
Mn/M2 - 3.9
lbf/in2 - 570
Defloculant Required - (3:1 Na2SiO3(C.100):Na2CO3) - 0.3
Water Absorption
1120C - 9.0
1220C - 1.00
Shrinkage Dry to Fired
1120C - 14.00
1220C - 17.50
Reflectance 464nm
1120C - 72
1220C - 57
Refractoriness
Cone - 33, 1730C
| Typecodes |
Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites. |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk