Description: Tennessee Ball Clay
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.20% | 0.01 | |
| K2O | 0.70% | 0.03 | |
| MgO | 0.20% | 0.02 | |
| Na2O | 0.10% | 0.01 | |
| TiO2 | 1.90% | 0.09 | |
| Al2O3 | 27.80% | 1.00 | |
| SiO2 | 58.20% | 3.55 | |
| Fe2O3 | 1.00% | 0.02 | |
| LOI | 9.90% | n/a | |
| C | 0.30% | n/a | |
| Oxide Weight | 330.58 | ||
| Formula Weight | 368.13 | ||
Particle Size (e.s.d.)
125 microns - 0.4
20 microns - 97
2 microns - 83
.5 microns - 59
Modulus of Rupture at 110C
Mn/M2 - 4.5
lbf/in2 - 650
Water Absorption
1120C - 23.0
1220C - 7.5
Shrinkage Dry to Fired
1120C - 7.5
1220C - 15.5
Refractoriness
Cone - 33, 1730C
| Typecodes |
Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites. |