Description: Tennessee Ball Clay
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.50% | 0.03 | |
| K2O | 0.70% | 0.03 | |
| MgO | 0.60% | 0.06 | |
| Na2O | 0.10% | 0.01 | |
| TiO2 | 1.20% | 0.06 | |
| Al2O3 | 27.40% | 1.00 | |
| SiO2 | 57.50% | 3.56 | |
| Fe2O3 | 2.60% | 0.06 | |
| LOI | 9.50% | n/a | |
| C | 0.20% | n/a | |
| Oxide Weight | 337.27 | ||
| Formula Weight | 373.50 | ||
Particle Size (e.s.d.)
125 microns - 0.2
20 microns - 97
2 microns - 87
.5 microns - 72
Modulus of Rupture at 110C
Mn/M2 - 15.5
lbf/in2 - 2250
Water Absorption
1120C - 15.0
1220C - 0.5
Shrinkage Dry to Fired
1120C - 8.0
1220C - 12.0
Refractoriness
Cone - 32, 1710C
| Typecodes |
Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites. |