Monthly Tech-Tip from Tony Hansen SignUp

No tracking! No ads!

3D Print a Test of the Beer Bottle Neck
3D Printing a Clay Cookie Cutter-Stamper
A 3-minute Mug with Plainsman Polar Ice
A Broken Glaze Meets Insight-Live and a Magic Material
Accessing Recipes from "Mid-Fire Glazes" book in Insight-Live
Adjusting the Thixotropy of an Engobe for Pottery
Analysing a Crazing, Cutlery-marking Glaze Using Insight-Live
Compare the Chemistry of Recipes Using Insight-Live
Connecting an External Image to Insight-Live Pictures
Convert a Cone 10 Glaze to Cone 6 Using Desktop Insight
Create a Synthetic Feldspar in Insight-Live
Creating a Cone 6 Oil-Spot Overglaze Effect
Creating Rules for Calcium Carbonate - Wollastonite Substitution
Design a Triangular Pottery Plate Block Mold in Fusion 360
Designing a Jigger Mold for a Bowl Using Fusion 360 CAD
Desktop Insight - Difficult Formula to Batch Calcuations
Desktop Insight 1A - Compare Theoretical and Real-World Feldspars
Desktop Insight 1B - Turn a Feldspar Into a Glaze
Desktop Insight 1C - Substitute Wollastonite for Whiting in Glazes
Desktop Insight 2 - Creating a Matte Glaze
Desktop Insight 3 - Dealing With Crazing
Desktop Insight 4 - Add a Native Material to MDT, Build a Glaze
Desktop Insight 5A - Glaze Formula to Batch Calculations
Desktop Insight MDT: Adding a Material
Desktop Insight: Maintain an MDT as a CSV File in Excel
Digitalfire Desktop INSIGHT Overview Part 1
Digitalfire Desktop INSIGHT Overview Part 2
Draw a propeller in Fusion 360 for use on an overhead propeller mixer
Drawing a Mug Handle Mold in Fusion 360
Enter a Recipe Into Insight-live
Entering Shrinkage/Porosity Data Into Insight-Live
Getting Frustrated With a 55% Gerstley Borate Glaze
How I Fixed a Settling Glaze Slurry Using Desktop Insight
How I Formulated a Cone 6 Silky Matte Glaze Using Insight-Live
How to Add Materials to the Desktop Insight MDT
How to Apply a White Slip to Terra Cotta Ware
How to Paste a Recipe Into Insight-live
Importing Data into Insight-live
Importing Desktop Insight Recipes to Insight-live
Importing Generic CSV Recipe Data into Insight-Live
Insight-Live Meets a Silica Deprived Glaze Recipe
Insight-Live Quick Overview
Liner Glazing a Stoneware Mug
Make a precision plaster mold for slip casting using Fusion 360 and 3D Printing
Make test bars to measure pottery clay physical properties
Making ceramic glaze flow test balls
Manually program your kiln or suffer glaze defects!
Mica and Feldspar Mine of MGK Minerals
Predicting Glaze Durability by Chemistry in Insight-Live
Preparing Pictures for Insight-live
Remove Gerstley Borate and Improve a Popular Cone 6 Clear Glaze
Replace Lithium Carbonate With Lithium Frit Using Insight-Live
Replacing 10% Gerstley Borate in a clear glaze
Signing Up at Insight-live.com
Signing-In at Insight-live.com
Slip cast a stoneware beer bottle
Subsitute Gerstley Borate in Floating Blue Using Desktop Insight
Substitute Ferro Frit 3134 For Another Frit
Substituting Custer Feldspar for Another in a Cone 10R Glaze Recipe
Substituting Materials by Weight: Why it does not work!
Substituting Nepheline Syenite for Soda Feldspar
Thixotropy and How to Gel a Ceramic Glaze
Use Insight-live to substitute materials in a recipe
Using Recipe Libraries With Desktop Insight

Subsitute Gerstley Borate in Floating Blue Using Desktop Insight

Use Desktop Insight to explore ways of calculating substitutes for Gerstley Borate in the popular Floating Blue cone 6 glaze recipe while maintaining or improving the other raw and fired properties of the glaze.

D. Desktop Insight


Click here to watch this at youtube.com or click here to go to our Youtube channel

In this video I will substitute Gerstley Borate for another boron source in the popular Floating Blue glaze recipe. The lesson demonstrates that the most practical way to deal with the GB issue is on a glaze-by-glaze basis, using an approach that maintains the chemistry of the glaze, evaluates the sources of boron in the light of the chemistry of GB but also its physical properties and their importance to the working properties of the glaze. The boron sourcing frit (Ferro Frit 3134) is tried first and proves to be unsuitable, then ulexite is employed and found to be an ideal substitute.

Lesson 6: Substituting Gerstley Borate in Floating Blue
Gerstleyborate.com, when frits are not suitable, ulexite, using phantom, static and added status with colorants and retotaling and static materials

1
Substituting Gerstley Borate in Floating Blue
Welcome. I am going to talk about substituting Gerstley Borate for another material in the popular floating blue glaze recipe.
Also Gerstleyborate.com, when frits are not suitable, ulexite, using phantom, static and added status with colorants and retotaling and static materials.
2
Gerstleyborate.com
Gerstley Borate has been a popular ingredient in raw glazes for many years. At digitalfire.com we author a website about this at gerstleyborate.com.
Recently it has gone through various perplexing cycles of becoming unavailable, then available again. More frequent changes in its behavior have accompanied this. The artware and pottery worlds have thus been absorbed in the pursuit of a substitute.
There is an better alternative. You can use INSIGHT to remove GB from your glazes and supply the lost oxides from other materials.
3
Floating blue glaze recipe
I will demonstrate replacement using the popular Floating Blue cone 6 glaze (this recipe has its own detailed page at gerstleyborate.com). I will replace the GB with another boron sourcing material.
I am going to be mentioning some techniques using INSIGHT that might not be totally clear unless you have watched some of the previous lessons.
4
Enter and duplicate the recipe
I have made sure the Lessons materials table is selected.
And have keyed floating blue into recipe 1 (I have left out the iron, cobalt and rutile, I am going work with the colorless base only).
Now I am going to click here to duplicate it into recipe 2 and make sure I have both recipes set to RO Unity calculation.
5
Replace Gerstley Borate with frit 3134
I have also removed the Gerstley Borate from recipe 2 by making sure its line was selected and clicking the line delete button.
I have also selected the next blank line in the recipe and added the same amount of Frit 3134.
Now if I click the MDT button to open the materials dialog you will notice that …
6
With this frit is a good choice
This frit contains no alumina, thus I can source alumina from kaolin to suspend the glaze. I need to think about this because it was the natural claylike nature of Gerstley Borate that kept the original glaze in suspension.
7
But this frit is not working
At first this frit seems like it could work. But it brings a lot of extra sodium so the nepheline, which is currently supplying the bulk of this, has to be dropped to compensate. This will create a balance that makes juggling the materials to match the oxides quite complex.
Notice I have also checked the KNaO box.
8
Turkish Ulexite is better
A better solution is to choose a material of more similar mineralogy and chemistry to Gerstley Borate. This is the substitutes page at GerstleyBorate.com.
Turkish Ulexite is imported into North America and other continents in large quantities for use the fiber glass industry.
If I click here I will be taken to a detail page at the Digitalfire Reference Database.
Let's try this ulexite.
9
Replacing GB with ulexite
I am going to replace the frit with 20 units of ulexite. Notice I have cleared the Label and am about to click Update.
10
Planning a strategy
Notice that the CaO and MgO are now lacking and the KNaO is high.
If I add materials to source the former, the latter should be pushed downward. Why? Because this is a unity formula, INSIGHT recalculates the fluxes to total one, if I increase one the other amounts drop.
Notice also that the SiO2 and Al2O3 are high. Increasing the total amount of flux is going to force their amounts downward for the same reason.
11
Matching CaO, MgO with whiting, talc
I have added talc to source MgO and Whiting to source CaO. I played with the amount of each (by incrementing and decrementing) to get the closest formula match on a recipe amount multiple of 1.
Notice the KNaO is just a little high…
12
Fine-tuning the new recipe
So now I will decrement the nepheline by 2 to match it up and then increase the kaolin by one to bring the Al2O3 back up to match.
Amazingly the silica does not need to be changed to adjust the SiO2.
Next, I am going to put the colorants into the recipe.
13
Assigning coloring oxides as phantom
Notice what happened here. When I entered this material I just typed “cobalt ox” assuming INSIGHT would find it in the materials database and expand the name. But this asterisk indicates that it did not find it. How do I know that? I can click here and this dialog explains what the status characters mean.
To get the name to look right I will edit this blank and update the line.
But that is not really a problem, I do not want coloring oxides in the formula anyway. So I am going to click this checkbox for these two lines and update also.
14
Using static colorants when retotaling a recipe
OK, these materials are not affecting the calculated formula anymore.
One more problem I want to deal with is this total. I would like to have a total of 107 and designate the coloring oxides as added materials.
But if I just recalculate to 107 the coloring oxide amounts are going to change. The solution is to first mark the three lines with static status. Static lines are ignored during retotal. Notice the new status characters.
15
Defining colorants as Added materials
I have chosen retotal from the Calc menu and specified 100 and then used Round Amounts in the Calc menu.
Here is the new total and the recipe. I should mention that the static status is not remembered with the recipe.
However added status is. I am going to set each of them as added using this checkbox, thus when I print the recipe they will be separated as such.
16
Fired samples: Improvements still needed
Take another look at the chemistry.
This glaze is very high in sodium and potassium and its calculated thermal expansion is likewise very high, that means crazing. However the high boron content appears to counteract this somewhat in practice. You can use INSIGHT to substitute some of the KNaO for another flux, but that might affect gloss.
Here are the fired samples. The Ulexite version has the same character, it just needs a cobalt/iron change for a little more color and a flow test to see if fluidity needs adjustment. The glaze slurry seems to work well also.
17
The End
This is yet another example of a problem that can only be effectively dealt with on the chemistry level.
Many people have struggled with this problem but doing it this way was quite simple, don’t you agree?
That is the end of this lesson.

Links

Materials Ulexite
A natural source of boron, it melts at a very low temperature to a clear glass.
Materials Gerstley Borate
Gerstley Borate was a natural source of boron for ceramic glazes. It was plastic and melted clear at 1750F. Now we need to replace it. How?
Materials Ferro Frit 3134
A frit with 23% B2O3. The most common of frits used in pottery in North America. Around the world, other companies make frits of equivalent chemistry.
Recipes G2826R - Floating Blue Cone 5-6 Original Glaze Recipe
Floating Blue is a classic cone 6 pottery glaze recipe from David Shaner. Because of the high Gerstley Borate content it is troublesome, difficult. But there are alternatives.
URLs https://digitalfire.com/videos
Tutorial Videos at Digitalfire
URLs https://gerstleyborate.com
GerstleyBorate.com - The best place for info on Gerstley Borate
This page is the gateway to the most comprehensive source of information about the material and what it actually is. It will get you on track to removing this troublesome material from your recipes and using frits instead.
Glossary Material Substitution
Material substitutions in ceramic glaze and body recipes must consider their chemistry, mineralogy and physical properties
Glossary Digitalfire Insight
A downloadable program for Windows, Mac, Linux for doing classic ceramic glaze chemistry. It has been used around the world since the early 1980s.
Glossary Glaze Gelling
Glaze slurries can gel if they contain soluble materials that flocculate the suspension. Gelling is a real problem since it requires water additions that increase shrinkage.
Typecodes Gerstley Borate Glaze Calculation examples
Examples of how we use glaze calculations (in an Insight-Live.com account) to replace Gerstley Borate with other materials, especially frits, in various glaze recipes. In doing so we take the opportunity to improve the recipe in other ways (e.g. reduce thermal expansion, improve slurry properties, reduce bubbling and crawling).

Here is what happens when a glaze has too much raw clay


A high clay glaze is cracking

This is an example of how a glaze that contains too much plastic clay has been applied too thick. It shrinks and cracks during drying and is guaranteed to crawl. This is raw Alberta Slip. To solve this problem you need to tune a mix of raw and roasted clay. Enough raw clay is needed to suspend the slurry and dry it to a hard surface, but enough calcine is needed to keep the shrinkage low enough that this cracking does not happen. Perhaps you have been using a glaze having a high percentage of clay and this does not happen - the reason is likely that the clay is not highly plastic.

Closeup of original floating blue recipe at cone 6


A much better Cone 6 Floating Blue


GR6-M Ravenscrag Cone 6 Floating Blue on Plainsman M340 buff stoneware. This glaze also has this variegated visual character on porcelain. Because it has the GR6 base recipe the slurry has very good working properties in the studio, it is a pleasure to use. This is an excellent showcase for the variegating mechanism of rutile.

Colemanite and what its decrepitation does in glazes


Decrepitation refers to a decomposition accompanied by scaling, delayering, even disintegration of the glaze layer. Moving rightward these glazes have increasing percentages of colemanite. At its worst (far right) the glaze is spattering off the sample and onto the kiln shelf. The others are crawling, first pulling away from the corners (far left) moving toward pulling away on the flat surfaces (center). Gerstley Borate and Ulexite, similar minerals, are far less likely to do this (but they have other serious issues also). A much better solution is to use frits to source the oxide B2O3 (easy to do in your account at Insight-live.com). Photos courtesy of Nigel Hicken.

By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy