Modified: 2009-05-23 11:16:49
Entirely opaque surface (crystals and ground)
Material | Amount |
---|---|
Ferro Frit 3110 | 46.00 |
Zinc Oxide | 18.00 |
Silica | 20.00 |
Dolomite | 9.00 |
Titanium Dioxide | 6.00 |
Talc | 1.00 |
100.00 |
An excellent "starter glaze" for new crystallieri.
Firing Schedules |
Shimbo Crystal Schedule 1
|
---|---|
Recipes |
GBCG1 - Frit 3110 Generic Base Crystalline Glaze
From Fara Shimbo Crystal Glaze book 2 |
Typecodes |
Crystalline Glaze Recipe Fara Shimbo
These are from Fara\'s Crystal Glazes book II. |
Glaze Color | Ground is completely opaque except where glaze pools or when applied very thickly to tiles. Crystals are tinted toward the golden and are sometimes quite yellow. Copper gives olive green and nickel is simply not a match, but cobalt, iron, manganese and most stains will color this glaze very well. Crystals are large and profuse. Matures at cone 9. |
---|