Monthly Tech-Tip | No tracking! No ads! |
Alternate Names: Guage Red
Description: High iron fireclay
Oxide | Analysis | Formula | |
---|---|---|---|
SiO2 | 40.80% | 2.47 | |
Al2O3 | 28.00% | 1.00 | |
Fe2O3 | 18.10% | 0.41 | |
TiO2 | 1.20% | 0.05 | |
MgO | 0.20% | 0.02 | |
K2O | 0.14% | 0.01 | |
LOI | 11.50% | n/a | |
Oxide Weight | 322.17 | ||
Formula Weight | 364.04 |
Replaces Carbondale Red and C-Red in 2021.
~5% retained on 200 mesh screen.
~8% quartz mineral.
Cone 04 water absorption: 23%
Cone 5 water absorption: 16%
Cone 10 water absorption: 11%
Cone 10R water absorption: 2%
In 2024 this is only being sold to selected customers, only about 800 tons per year are being mined.