Oxide | Analysis | Formula | |
---|---|---|---|
CaO | 0.05% | 0.00 | |
K2O | 0.15% | 0.00 | |
MgO | 0.02% | 0.00 | |
Na2O | 0.21% | 0.01 | |
TiO2 | 1.58% | 0.05 | |
Al2O3 | 37.85% | 1.00 | |
SiO2 | 45.68% | 2.05 | |
Fe2O3 | 0.74% | 0.01 | |
LOI | 13.72% | ||
Oxide Weight | 232.51 | ||
Formula Weight | 269.48 |
Wilclay WC is a clean, high quality, white-firing airfloated kaolin especially selected for the whitewares segment of the ceramic industries. The clay has an intermediately fine particle size and has relatively high plasticity.
Moisture, Maximum %: 2.0
Median Particle Size, microns: .78
pH (28% solids): 4.5-7.0
CEC, Meq/100 gm.: 7.0
Particle size: % Finer Than
20 microns: 98
10: 94
5: 89
2: 75
1: 63
0.5: 45
Materials | Kaolin |
---|---|
Typecodes |
Kaolin
Pure clay mineral, there are many brand names of varying purity and iron content. |