Wilclay CR Kaolin

WHITE AIRFLOATED KAOLIN

OxideAnalysisFormula
CaO0.05%0.002
MgO0.02%0.001
K2O0.15%0.004
Na2O0.21%0.009
TiO21.62%0.055
Al2O337.80%1.000
SiO245.60%2.047
Fe2O30.85%0.014
LOI13.70
Oxide Weight232.87
Formula Weight269.84
If this formula is not unified correctly please contact us.

Wilklay CR is a clean, high quality, white-firing airfloated kaolin especially selected for the ceramic and refractories industries. The clay has an intermediately fine particle size and has relatively high plasticity.

Moisture, Maximum %: 2.0
Median Particle Size, microns: .78
pH (28% solids): 4.5-7.0
CEC, Meq/100 gm.: 6.5

Particle size: % Finer Than
20 microns: 98
10: 93
5: 86
2: 72
1: 62
0.5: 43


Out Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="Wilclay CR Kaolin" descrip="WHITE AIRFLOATED KAOLIN" searchkey="" loi="13.70" casnumber="95077-05-7"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.050" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.020" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="0.150" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.210" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="1.620" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="37.800" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="45.600" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="0.850" tolerance=""/> </oxides> <volatiles> <volatile symbol="LOI" name="Loss on Ignition" percent="13.700" tolerance=""/> </volatiles> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved