USAKOS Wollastonite

OxideAnalysisFormula
CaO46.00%0.990
MgO0.20%0.006
K2O0.05%0.001
Na2O0.15%0.003
P2O50.05%0.000
TiO20.13%0.002
Al2O30.20%0.002
SiO253.00%1.065
Fe2O30.15%0.001
LOI1.85
Oxide Weight120.65
Formula Weight122.93
If this formula is not unified correctly please contact us.

Hardness 4.5
PH 9.9
Moisture content 0.02%
Sintering temperature 991-1196=B0C
Melting point 1540=B0C
Coefficient of expansion 6.5 x 10-6 cm/cm/=B0C
Water solubility 0.0095g/100.c.c
Aspect ration 2:1
Particle size distribution depends on the size that the product is milled to.


Out Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="USAKOS Wollastonite" descrip="" searchkey="" loi="0.00" casnumber="9056-30-8"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="46.000" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.200" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="0.050" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.150" tolerance=""/> <oxide symbol="P2O5" name="Phosphorus Pentoxide" status="" percent="0.050" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="0.130" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="0.200" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="53.000" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="0.150" tolerance=""/> </oxides> <volatiles> <volatile symbol="LOI" name="Loss on Ignition" percent="1.850" tolerance=""/> </volatiles> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved