Thomas Ball Clay

Oxide Analysis Formula
CaO 0.06% 0.00
K2O 0.40% 0.02
MgO 0.20% 0.02
Na2O 0.08% 0.00
TiO2 1.60% 0.08
Al2O3 26.50% 1.00
SiO2 59.40% 3.80
Fe2O3 1.02% 0.02
LOI10.60%
Oxide Weight 343.57
Formula Weight 384.30

Notes

Crude Color: Brown
Dry M.O.R. (psi 50% clay/50% flint, cast bars): 511
Wet Sieve Residue, +200 mesh (%): 0.31
Water of Plasticity (%): 36
Linear Dry Shrinkage (%): 7.26
Solubles Sulfates (ppm): 283
Filtration (ml): 26
Specific Surface Area (sq meters per gram): 19.8
CEC/MBI (meq/100 ml): 10.5
pH: 5.3
PCE: 31

Firing Shrinkage (%) Cone 04: 5.9 Cone 3: 7.0 Cone 11: 8.0
Absorption (%) 16.2 10.8 4.0

Particle Size (% finer than):
50 microns: 100
20: 96
10: 93
5: 85
1: 65
0.5: 54

Related Information

Links

Materials Cooley No. 2 Ball Clay
Materials Ball Clay
Suppliers Old Hickory
Suppliers Cooley Clay Co.
Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

By Tony Hansen


Tell Us How to Improve This Page

Or ask a question and we will alter this page to better answer it.

Email Address

Name

Subject

Message


Upload picture


Copyright 2008, 2015, 2017 https://digitalfire.com, All Rights Reserved