Tapper's Clay

REFRACTORY CLAY

OxideAnalysisFormula
CaO0.11%0.013
MgO0.16%0.027
K2O0.80%0.057
Na2O0.11%0.012
TiO20.83%0.070
Al2O315.21%1.000
SiO259.11%6.596
Fe2O30.89%0.037
LOI7.70
Oxide Weight517.85
Formula Weight561.05
If this formula is not unified correctly please contact us.

Physical Properties:

Temp Bulk Cold Crushing M.O.R. Linear
(F) Density Strength (psi) (psi) Change %

230 123.6 455 285
1000 115.5 977 244 +0.47
1500 114.8 1416 268 +0.49
2000 118.6 2059 585 -1.49


Out Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="Tapper's Clay" descrip="REFRACTORY CLAY" searchkey="" loi="7.70" casnumber="70694-09-6"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.110" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.160" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="0.800" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.110" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="0.830" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="15.210" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="59.110" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="0.890" tolerance=""/> </oxides> <volatiles> <volatile symbol="LOI" name="Loss on Ignition" percent="7.700" tolerance=""/> </volatiles> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved