Sanblend 75 Ball Clay

Noodled refined Devon ball clay

OxideAnalysisFormula
CaO0.20%0.012
MgO0.30%0.025
K2O2.20%0.078
Na2O0.30%0.016
TiO21.20%0.050
Al2O330.50%1.000
SiO252.40%2.916
Fe2O31.00%0.021
C2.50
LOI11.90
Oxide Weight294.63
Formula Weight344.19
If this formula is not unified correctly please contact us.

Particle Size (e.s.d.)
125 microns - 0.20
10 microns - 97
2 microns - 82
1 microns - 72
Modulus of Rupture at 110C
Mn/M2 - 7.6
lbf/in2 - 1110
Defloculant Required - (3:1 Na2SiO3(C.100):Na2CO3) - 0.2
Water Absorption
1120C - 2.0
1220C - 0.50
Shrinkage Dry to Fired
1120C - 12.50
1220C - 14.00
Reflectance 464nm
1120C - 67
1220C - 52
Refractoriness
Cone - 33, 1730C


Out Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="Sanblend 75 Ball Clay" descrip="Noodled refined Devon ball clay" searchkey="" loi="0.00" casnumber="70694-09-6"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.200" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.300" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="2.200" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.300" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="1.200" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="30.500" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="52.400" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="1.000" tolerance=""/> </oxides> <volatiles> <volatile symbol="C" name="Carbon" percent="2.500" tolerance=""/> <volatile symbol="LOI" name="Loss on Ignition" percent="11.900" tolerance=""/> </volatiles> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved