Sagger XX Ball Clay

Alternate Names: XX Sagger, XX Sagger Ball Clay, Saggar

OxideAnalysisFormula
CaO0.50%0.031
MgO0.30%0.026
K2O0.89%0.033
Na2O0.30%0.017
TiO21.71%0.075
Al2O329.17%1.000
SiO256.73%3.301
Fe2O30.69%0.015
LOI9.71
Oxide Weight315.72
Formula Weight349.67
If this formula is not unified correctly please contact us.
PCE - Pyrometric Cone Equivalent 32.5
WABS - Water absorption Cone 5: 11% cone 10: 3%
UPSD - Ultimate Particle Size Distribution 20 microns: 99% 10: 97% 8: 94% 5: 88% 3: 79% 2: 73% 1: 60% 0.5: 45%

A fine grained secondary clay which fires to a light cream with 13% shrinkage at cone 10. This ball clay is considered to be very effective in salt firing and it is claimed that it works well in flashing (i.e. wood firing).


Out Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="Sagger XX Ball Clay" descrip="" searchkey="XX Sagger, XX Sagger Ball Clay, Saggar" loi="0.00" casnumber="70694-09-6"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.500" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.300" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="0.890" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.300" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="1.710" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="29.170" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="56.730" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="0.690" tolerance=""/> </oxides> <volatiles> <volatile symbol="LOI" name="Loss on Ignition" percent="9.710" tolerance=""/> </volatiles> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved