Rex Ball Clay

Tennessee Ball Clay

OxideAnalysisFormula
CaO0.10%0.006
MgO0.30%0.026
K2O1.60%0.059
Na2O0.10%0.006
TiO21.90%0.083
Al2O329.30%1.000
SiO256.40%3.267
Fe2O30.80%0.017
C0.10
LOI9.50
Oxide Weight315.05
Formula Weight348.51
If this formula is not unified correctly please contact us.

Particle Size (e.s.d.)
125 microns - 0.3
20 microns - 97
2 microns - 65
.5 microns - 35
Modulus of Rupture at 110C
Mn/M2 - 2.2
lbf/in2 - 320
Water Absorption
1120C - 15.0
1220C - 4.0
Shrinkage Dry to Fired
1120C - 8.0
1220C - 12.0
Refractoriness
Cone - 32, 1710C


Out Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="Rex Ball Clay" descrip="Tennessee Ball Clay" searchkey="" loi="0.00" casnumber="70694-09-6"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.100" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.300" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="1.600" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.100" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="1.900" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="29.300" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="56.400" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="0.800" tolerance=""/> </oxides> <volatiles> <volatile symbol="C" name="Carbon" percent="0.100" tolerance=""/> <volatile symbol="LOI" name="Loss on Ignition" percent="9.500" tolerance=""/> </volatiles> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved