WBB Devon Ball Clay Group 4

OxideAnalysisFormula
CaO0.20%0.016
MgO0.30%0.032
K2O2.20%0.102
Na2O0.30%0.021
TiO21.40%0.076
Al2O323.40%1.000
SiO264.90%4.707
Fe2O30.80%0.022
C0.20
LOI6.50
Oxide Weight407.56
Formula Weight436.83
If this formula is not unified correctly please contact us.

Particle Size (e.s.d.)
125 microns - 0.60
10 microns - 96
2 microns - 75
1 microns - 65
Modulus of Rupture at 110C
Mn/M2 - 4.6
lbf/in2 - 670
Defloculant Required - (3:1 Na2SiO3(C.100):Na2CO3) - 0.5
Water Absorption
1120C - 1.0
1220C - 0.50
Shrinkage Dry to Fired
1120C - 11.50
1220C - 12.50
Reflectance 464nm
1120C - 64
1220C - 47
Refractoriness
Cone - 31, 1690C


Out Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="RBV Ball Clay" descrip="WBB Devon Ball Clay Group 4" searchkey="" loi="0.00" casnumber="70694-09-6"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.200" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.300" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="2.200" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.300" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="1.400" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="23.400" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="64.900" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="0.800" tolerance=""/> </oxides> <volatiles> <volatile symbol="C" name="Carbon" percent="0.200" tolerance=""/> <volatile symbol="LOI" name="Loss on Ignition" percent="6.500" tolerance=""/> </volatiles> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved