Pyrofrac 0304

Oxide Analysis Formula
K2O 0.45% 0.03
Na2O 0.45% 0.05
TiO2 0.40% 0.04
Al2O3 14.50% 1.00
SiO2 77.30% 9.05
Fe2O3 1.00% 0.04
H2O5.90%
Oxide Weight 661.94
Formula Weight 703.45

Notes

Used in structural clay coatings, refractory formulations, whiteware ceramics, art pottery to
increase refractoriness, reduce shrinkage, and widen firing range.
This material is made by crushing & screening of selectively mined andalusite/pyrophyllite/sericite ores
with heavy media separation.

Related Information

Links

Materials Andalusite
Materials Pyrophyllite
Materials Alkatrol
Materials Pyrofrac
Materials Seriphyl
Suppliers RESCO Products

Data

Bulk Density lbs/cu. ft. (Packed)100
Pyrometric Cone Equivalent20
Sieve Analysis Dry+20 mesh: 0.1 +50 mesh: 12.0 +70 mesh: 16.0 +100 mesh: 20.0 +200 mesh: 26.5 +325 mesh: 14.0
Density (Specific Gravity)2.6

By Tony Hansen


Tell Us How to Improve This Page

Or ask a question and we will alter this page to better answer it.

Email Address

Name

Subject

Message


Upload picture


Copyright 2008, 2015, 2017 https://digitalfire.com, All Rights Reserved