OxideAnalysisFormula
CaO0.04%0.002
MgO0.22%0.015
K2O1.60%0.046
Na2O0.06%0.003
TiO20.30%0.010
Al2O337.50%1.000
SiO247.50%2.150
Fe2O30.65%0.011
LOI12.30
Oxide Weight239.01
Formula Weight272.53
If this formula is not unified correctly please contact us.

Particle Size Distribution:
>53 microns: 0.1 max
>10 microns: 8
<2 microns: 61

Modulus of Rupture, Kgf/cm2:
At 80% Relative Humidity: 10.0
Dried at 110C: 21.0

Casting Rate @ 65% solids (mm2/min): 0.35
% P84 Deflocculant Required for 5 Poise Slip: 0.4

1180C 1280C
Fired Absorption: 20% 11%
Fired Shrinkage: 7% 11.5%
Brightness: 90 88


Out Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="Pleyber G" descrip="" searchkey="" loi="0.00" casnumber=""> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.040" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.220" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="1.600" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.060" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="0.300" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="37.500" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="47.500" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="0.650" tolerance=""/> </oxides> <volatiles> <volatile symbol="LOI" name="Loss on Ignition" percent="12.300" tolerance=""/> </volatiles> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved