Pemco Frit PC-4X63

Low flux high boron/silica low expansion frit

OxideAnalysisFormula
Li2O1.50%0.666
K2O0.10%0.014
Na2O1.50%0.320
Al2O37.00%0.908
B2O320.00%3.801
SiO269.90%15.386
Oxide Weight1322.91
Formula Weight1322.91
If this formula is not unified correctly please contact us.
COLE - Co-efficient of Linear Expansion 3.7 x 10-6
MLRG - Frit Melting Range (C) 1350C

Suggested recipe cone 03 gas firing:
Frit 93%
Ball Clay 7
Black Glaze Stain 5
CMC 0.2

It appears the melting temperature of 1350C is overstated, it obviously melts earlier.


Out Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="Pemco Frit PC-4X63" descrip="Low flux high boron/silica low expansion frit" searchkey="" loi="0.00" casnumber=""> <oxides> <oxide symbol="Li2O" name="Lithium Oxide, Lithia" status="" percent="1.500" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="0.100" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="1.500" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="7.000" tolerance=""/> <oxide symbol="B2O3" name="Boric Oxide" status="" percent="20.000" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="69.900" tolerance=""/> </oxides> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved