Pemco Frit P-1701

LEADLESS FRIT

Alternate Names: Frit 1701, Frit P1701

OxideAnalysisFormula
CaO4.70%0.462
Li2O0.40%0.074
K2O1.00%0.059
Na2O3.90%0.347
SrO1.10%0.059
Al2O39.10%0.492
B2O327.00%2.139
SiO252.80%4.845
Oxide Weight551.45
Formula Weight551.45
If this formula is not unified correctly please contact us.
COLE - Co-efficient of Linear Expansion 5.40
GSPT - Frit Softening Point 1490F
MLRG - Frit Melting Range (C) 1460-1550F
IFP - I.F.P. (celsius) 612C

All-fritted glaze for high alumina bodies firing in the range of 1600-1800F.


Out Bound Links

In Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="Pemco Frit P-1701" descrip="LEADLESS FRIT" searchkey="Frit 1701, Frit P1701" loi="0.00" casnumber="65997-18-4"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="4.700" tolerance=""/> <oxide symbol="Li2O" name="Lithium Oxide, Lithia" status="" percent="0.400" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="1.000" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="3.900" tolerance=""/> <oxide symbol="SrO" name="Strontium Oxide, Strontia" status="" percent="1.100" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="9.100" tolerance=""/> <oxide symbol="B2O3" name="Boric Oxide" status="" percent="27.000" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="52.800" tolerance=""/> </oxides> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved