LM1/S Ball Clay

Devon Standard Ball Clay

OxideAnalysisFormula
CaO0.20%0.013
MgO0.30%0.027
K2O1.80%0.068
Na2O0.20%0.012
TiO21.20%0.054
Al2O328.60%1.000
SiO256.20%3.335
Fe2O31.00%0.022
C1.10
LOI10.60
Oxide Weight319.20
Formula Weight361.49
If this formula is not unified correctly please contact us.

Particle Size (e.s.d.)
125 microns - 0.60
10 microns - 96
2 microns - 78
1 microns - 68
Modulus of Rupture at 110C
Mn/M2 - 3.8
lbf/in2 - 550
Defloculant Required - (3:1 Na2SiO3(C.100):Na2CO3) - 0.4
Water Absorption
1120C - 8.0
1220C - 0.50
Shrinkage Dry to Fired
1120C - 13.00
1220C - 15.50
Reflectance 464nm
1120C - 74
1220C - 52
Refractoriness
Cone - 31, 1690C


Out Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="LM1/S Ball Clay" descrip="Devon Standard Ball Clay" searchkey="" loi="0.00" casnumber="70694-09-6"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.200" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.300" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="1.800" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.200" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="1.200" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="28.600" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="56.200" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="1.000" tolerance=""/> </oxides> <volatiles> <volatile symbol="C" name="Carbon" percent="1.100" tolerance=""/> <volatile symbol="LOI" name="Loss on Ignition" percent="10.600" tolerance=""/> </volatiles> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved