Kaolin SP

WBB Devon Ball Clay Group 2

OxideAnalysisFormula
CaO0.20%0.011
MgO0.30%0.023
K2O1.50%0.048
Na2O0.10%0.005
TiO20.90%0.034
Al2O333.70%1.000
SiO249.20%2.478
Fe2O31.20%0.023
C2.60
LOI12.90
Oxide Weight263.63
Formula Weight311.98
If this formula is not unified correctly please contact us.

Particle Size (e.s.d.)
125 microns - 0.50
10 microns - 98
2 microns - 83
1 microns - 73
Modulus of Rupture at 110C
Mn/M2 - 5.2
lbf/in2 - 750
Defloculant Required - (3:1 Na2SiO3(C.100):Na2CO3) - 0.7
Water Absorption
1120C - 5.5
1220C - 0.50
Shrinkage Dry to Fired
1120C - 14.50
1220C - 16.50
Reflectance 464nm
1120C - 79
1220C - 63
Refractoriness
Cone - 33, 1730C


Out Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="Kaolin SP" descrip="WBB Devon Ball Clay Group 2" searchkey="" loi="0.00" casnumber="70694-09-6"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.200" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.300" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="1.500" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.100" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="0.900" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="33.700" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="49.200" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="1.200" tolerance=""/> </oxides> <volatiles> <volatile symbol="C" name="Carbon" percent="2.600" tolerance=""/> <volatile symbol="LOI" name="Loss on Ignition" percent="12.900" tolerance=""/> </volatiles> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved