Kaolin 115

Alternate Names: Kaolen 115

OxideAnalysisFormula
CaO0.09%0.006
MgO0.29%0.026
K2O0.12%0.005
Na2O0.13%0.008
TiO20.43%0.019
Al2O328.17%1.000
SiO259.46%3.582
Fe2O30.51%0.012
SO40.65
LOI10.80
Oxide Weight322.98
Formula Weight364.75
If this formula is not unified correctly please contact us.
WABS - Water absorption 1000C: 17.5% 1100C: 17% 1200C: 14% 1250C: 12.5%
FSHR - Firing Shrinkage 1000C: 8.0% 1100C: 9% 1200C: 11% 1250C: 12.5%

Available in run-of-mine, 25mm and 50mm sizes.


Out Bound Links

In Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="Kaolin 115" descrip="" searchkey="Kaolen 115" loi="0.00" casnumber="95077-05-7"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.090" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.290" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="0.120" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.130" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="0.430" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="28.170" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="59.460" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="0.510" tolerance=""/> </oxides> <volatiles> <volatile symbol="SO4" name="Sulfate" percent="0.650" tolerance=""/> <volatile symbol="LOI" name="Loss on Ignition" percent="10.800" tolerance=""/> </volatiles> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved