HVA/R Ball Clay

Oxide Analysis Formula
CaO 0.20% 0.01
K2O 2.60% 0.11
MgO 0.30% 0.03
Na2O 0.40% 0.02
TiO2 1.50% 0.07
Al2O3 26.70% 1.00
SiO2 60.30% 3.83
Fe2O3 0.90% 0.02
LOI7.10%
C0.10%
Oxide Weight 354.90
Formula Weight 382.43

Notes

Particle Size (e.s.d.)
125 microns - 0.60
10 microns - 96
2 microns - 75
1 microns - 65
Modulus of Rupture at 110C
Mn/M2 - 4.6
lbf/in2 - 670
Defloculant Required - (3:1 Na2SiO3(C.100):Na2CO3) - 0.8
Water Absorption
1120C - 1.0
1220C - 0.50
Shrinkage Dry to Fired
1120C - 11.50
1220C - 12.50
Reflectance 464nm
1120C - 63
1220C - 37
Refractoriness
Cone - 31, 1690C

Related Information

Links

Materials Ball Clay
Suppliers WBB
Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

By Tony Hansen


Tell Us How to Improve This Page

Or ask a question and we will alter this page to better answer it.

Email Address

Name

Subject

Message


Upload picture


Copyright 2008, 2015, 2017 https://digitalfire.com, All Rights Reserved