G200 Old Blend Feldspar

Alternate Names: MFEL S3470 Blend

OxideAnalysisFormula
CaO1.00%0.100
K2O10.50%0.627
Na2O3.00%0.272
Al2O318.20%1.004
SiO266.80%6.256
Fe2O30.08%0.003
LOI0.20
Oxide Weight560.45
Formula Weight561.58
If this formula is not unified correctly please contact us.

To be as similar as possible to the old G-200 feldspar, Laguna Clays blended 3 parts Minspar and 7 parts G-200 HP to produce this material.
However G-200HP was then discontinued so Laguna Clays began importing Mahavir Feldspar from India.

Old Blend Feldspar. What is that?

Old Blend Feldspar. What is that?

Laguna Clay sells a substitute for the no-longer-available G200 feldspar. G200 HP is higher in K2O and lower in CaO than G200, Minspar is an ideal addition since it's K2O is much lower and CaO much higher. A 7:3 G200HP:Minspar mix produces a chemistry that is remarkably close (on paper) to G200. They label this blend "Old Blend". They also list a product called "New Potash" in their pricelist, that is G200 HP.

Out Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="G200 Old Blend Feldspar" descrip="" searchkey="MFEL S3470 Blend" loi="0.00" casnumber=""> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="1.000" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="10.500" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="3.000" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="18.200" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="66.800" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="0.080" tolerance=""/> </oxides> <volatiles> <volatile symbol="LOI" name="Loss on Ignition" percent="0.200" tolerance=""/> </volatiles> </material>