FT-K Clay

Westerwald, Germany - Plastic Clay

OxideAnalysisFormula
CaO0.20%0.020
MgO0.10%0.014
K2O1.80%0.108
Na2O0.20%0.018
TiO21.30%0.092
Al2O318.10%1.000
SiO272.10%6.761
Fe2O31.00%0.035
C0.20
LOI5.10
Oxide Weight534.23
Formula Weight564.13
If this formula is not unified correctly please contact us.

Raw Color - LIGHT GREY-LIGHT CREAM
Particle Size (e.s.d.)
125 microns - 0.5
63 microns - 3.7
20 microns - 86
2 microns - 55
.5 microns - 40
Modulus of Rupture at 110C
Mn/M2 - 4.7
lbf/in2 - 680
Water Absorption
1120C - 7.0
1220C - 1
Shrinkage Dry to Fired
1120C - 5.0
1220C - 7.0
Refractoriness
Cone - 29, 1650C
Plastic Index - 398
PF NO. - 26.4


Out Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="FT-K Clay" descrip="Westerwald, Germany - Plastic Clay" searchkey="" loi="5.30" casnumber="70694-09-6"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.200" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.100" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="1.800" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.200" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="1.300" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="18.100" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="72.100" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="1.000" tolerance=""/> </oxides> <volatiles> <volatile symbol="C" name="Carbon" percent="0.200" tolerance=""/> <volatile symbol="LOI" name="Loss on Ignition" percent="5.100" tolerance=""/> </volatiles> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved