FT-163 Clay

Westerwald, Germany - Plastic Clay

OxideAnalysisFormula
CaO0.10%0.013
MgO0.20%0.037
K2O1.20%0.094
Na2O0.20%0.024
TiO21.40%0.130
Al2O313.80%1.000
SiO278.50%9.654
Fe2O30.60%0.028
C0.10
LOI4.00
Oxide Weight709.57
Formula Weight739.90
If this formula is not unified correctly please contact us.

Raw Color - WHITE-LIGHT GREY
Particle Size (e.s.d.)
125 microns - 4.6
63 microns - 9.5
20 microns - 60
2 microns - 37
.5 microns - 29
Modulus of Rupture at 110C
Mn/M2 - 2.4
lbf/in2 - 340
Water Absorption
1120C - 12.0
1220C - 8
Shrinkage Dry to Fired
1120C - 3.0
1220C - 6.0
Refractoriness
Cone - 31, 1690C
Plastic Index - 489
PF NO. - 23.2


Out Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="FT-163 Clay" descrip="Westerwald, Germany - Plastic Clay" searchkey="" loi="4.10" casnumber="70694-09-6"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.100" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.200" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="1.200" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.200" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="1.400" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="13.800" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="78.500" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="0.600" tolerance=""/> </oxides> <volatiles> <volatile symbol="C" name="Carbon" percent="0.100" tolerance=""/> <volatile symbol="LOI" name="Loss on Ignition" percent="4.000" tolerance=""/> </volatiles> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved