Ferro Frit 3248

Leadless calcium potassium borosilicate frit

OxideAnalysisFormula
CaO5.20%0.382
MgO1.99%0.203
K2O7.00%0.306
Na2O1.63%0.108
Al2O315.10%0.610
B2O34.70%0.278
SiO264.39%4.415
Oxide Weight412.12
Formula Weight412.12
If this formula is not unified correctly please contact us.
COLE - Co-efficient of Linear Expansion 8.60
MLRG - Frit Melting Range (C) 1900F

Out Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="Ferro Frit 3248" descrip="Leadless calcium potassium borosilicate frit" searchkey="" loi="0.00" casnumber="65997-18-4"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="5.200" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="1.990" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="7.000" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="1.630" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="15.100" tolerance=""/> <oxide symbol="B2O3" name="Boric Oxide" status="" percent="4.700" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="64.390" tolerance=""/> </oxides> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved