Clay 261

OxideAnalysisFormula
CaO0.21%0.012
MgO0.38%0.030
K2O0.61%0.021
Na2O0.08%0.004
TiO20.78%0.031
Al2O332.21%1.000
SiO250.87%2.680
Fe2O32.43%0.048
SO40.16
LOI12.19
Oxide Weight277.31
Formula Weight316.38
If this formula is not unified correctly please contact us.
SADR - Sieve Analysis Dry > 41 micron: 0% > 30 micron: 0.39% > 20 micron: 2.02% > 10 micron: 24.4% < 3 micron: 28.49%
DS - Dry Strength (kgf/cm2) 16.51
FSHR - Firing Shrinkage 1150C: 6.33% 1200C: 6.73% 1250C: 7.39% 1325C: 8.39%

Out Bound Links

In Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="Clay 261" descrip="" searchkey="" loi="0.00" casnumber="70694-09-6"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.210" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.380" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="0.610" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.080" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="0.780" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="32.210" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="50.870" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="2.430" tolerance=""/> </oxides> <volatiles> <volatile symbol="SO4" name="Sulfate" percent="0.160" tolerance=""/> <volatile symbol="LOI" name="Loss on Ignition" percent="12.190" tolerance=""/> </volatiles> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved