Clay 244

Alternate Names: Kil 244

OxideAnalysisFormula
CaO0.27%0.018
MgO0.60%0.057
K2O2.17%0.087
Na2O0.04%0.002
TiO20.80%0.038
Al2O326.87%1.000
SiO259.12%3.734
Fe2O31.54%0.037
SO40.35
LOI8.45
Oxide Weight347.00
Formula Weight380.48
If this formula is not unified correctly please contact us.
SADR - Sieve Analysis Dry > 41 micron: 0% > 30 micron: 0.68% > 20 micron: 3.01% > 10 micron: 15.37% < 3 micron: 44.67%
DS - Dry Strength (kgf/cm2) 25.23
WABS - Water absorption 1150C: 2.0% 1200C: 1.75% 1250C: 1.0% 1325C: 0%
FSHR - Firing Shrinkage 1150C: 10.0% 1200C: 11.0% 1250C: 11.5% 1325C: 12.5%

Out Bound Links

In Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="Clay 244" descrip="" searchkey="Kil 244" loi="0.00" casnumber="70694-09-6"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.270" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.600" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="2.170" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.040" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="0.800" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="26.870" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="59.120" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="1.540" tolerance=""/> </oxides> <volatiles> <volatile symbol="SO4" name="Sulfate" percent="0.350" tolerance=""/> <volatile symbol="LOI" name="Loss on Ignition" percent="8.450" tolerance=""/> </volatiles> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved