Clay 232

Alternate Names: Kil 232

OxideAnalysisFormula
CaO0.12%0.008
MgO0.64%0.062
K2O2.45%0.101
Na2O0.49%0.031
TiO20.90%0.044
Al2O326.15%1.000
SiO257.57%3.736
Fe2O32.49%0.061
SO40.45
Organics0.27
LOI8.69
Oxide Weight354.21
Formula Weight391.00
If this formula is not unified correctly please contact us.
SADR - Sieve Analysis Dry < 212 micron: 99.53% < 150 micron: 99.3% < 106 micron: 98.83% < 63 micron: 97.68% < 45 micron:
DS - Dry Strength (kgf/cm2) 45.0
WABS - Water absorption 1050C: 18.0% 1100C: 14.0% 1150C: 8.0% 1200C: 2.0% 1250C: 0.5%
FSHR - Firing Shrinkage 1050C: 3.0% 1100C: 7.0% 1150C: 11.0% 1200C: 16.0% 1250C: 18.0%

Out Bound Links

In Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="Clay 232" descrip="" searchkey="Kil 232" loi="0.00" casnumber="70694-09-6"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.120" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.640" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="2.450" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.490" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="0.900" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="26.150" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="57.570" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="2.490" tolerance=""/> </oxides> <volatiles> <volatile symbol="SO4" name="Sulfate" percent="0.450" tolerance=""/> <volatile symbol="Organics" name="" percent="0.270" tolerance=""/> <volatile symbol="LOI" name="Loss on Ignition" percent="8.690" tolerance=""/> </volatiles> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved