Clay 222

Alternate Names: Kil 222

OxideAnalysisFormula
CaO0.30%0.019
MgO0.33%0.030
K2O2.34%0.090
Na2O0.22%0.013
TiO20.60%0.027
Al2O328.08%1.000
SiO255.83%3.374
Fe2O32.28%0.052
SO40.53
Organics0.40
C0.23
LOI10.02
Oxide Weight326.85
Formula Weight367.99
If this formula is not unified correctly please contact us.
SADR - Sieve Analysis Dry < 212 micron: 98.9% < 150 micron: 98.0% < 106 micron: 97.1% < 63 micron: 94.7% < 45 micron: 93.
DS - Dry Strength (kgf/cm2) 45.0
WABS - Water absorption 1050C: 20.0% 1100C: 16.5% 1150C: 8.0% 1200C: 5.0% 1250C: 3.0%
FSHR - Firing Shrinkage 1050C: 2.0% 1100C: 5.0% 1150C: 9.0% 1200C: 12.0% 1250C: 14.0%

Out Bound Links

In Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="Clay 222" descrip="" searchkey="Kil 222" loi="0.00" casnumber="70694-09-6"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.300" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.330" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="2.340" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.220" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="0.600" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="28.080" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="55.830" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="2.280" tolerance=""/> </oxides> <volatiles> <volatile symbol="SO4" name="Sulfate" percent="0.530" tolerance=""/> <volatile symbol="Organics" name="" percent="0.400" tolerance=""/> <volatile symbol="C" name="Carbon" percent="0.230" tolerance=""/> <volatile symbol="LOI" name="Loss on Ignition" percent="10.020" tolerance=""/> </volatiles> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved