Clay 220

Alternate Names: Kil 220

OxideAnalysisFormula
CaO0.10%0.009
MgO0.60%0.071
K2O2.00%0.102
Na2O0.10%0.008
TiO26.70%0.402
Al2O321.30%1.000
SiO266.80%5.323
Fe2O31.80%0.054
SO40.20
Organics0.16
C0.09
LOI6.70
Oxide Weight476.00
Formula Weight512.65
If this formula is not unified correctly please contact us.
SADR - Sieve Analysis Dry < 212 micron: 99.0% < 150 micron: 98.1% < 106 micron: 96.7% < 63 micron: 92.5% < 45 micron: 89.
DS - Dry Strength (kgf/cm2) 32.0
WABS - Water absorption 1050C: 17% 1100C: 15% 1150C: 11% 1200C: 7% 1250C: 3%
FSHR - Firing Shrinkage 1100C: 3% 1150C: 6% 1200C: 9% 1250C: 10%

Out Bound Links

In Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="Clay 220" descrip="" searchkey="Kil 220" loi="4.00" casnumber="70694-09-6"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.100" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.600" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="2.000" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.100" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="6.700" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="21.300" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="66.800" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="1.800" tolerance=""/> </oxides> <volatiles> <volatile symbol="SO4" name="Sulfate" percent="0.200" tolerance=""/> <volatile symbol="Organics" name="" percent="0.160" tolerance=""/> <volatile symbol="C" name="Carbon" percent="0.090" tolerance=""/> <volatile symbol="LOI" name="Loss on Ignition" percent="6.700" tolerance=""/> </volatiles> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved