Clay 215

Alternate Names: Kil 215

OxideAnalysisFormula
CaO0.20%0.015
MgO0.60%0.061
K2O1.90%0.082
Na2O0.20%0.013
TiO20.60%0.031
Al2O325.00%1.000
SiO259.50%4.039
Fe2O32.20%0.056
SO40.57
Organics0.36
C0.21
LOI8.90
Oxide Weight368.02
Formula Weight409.09
If this formula is not unified correctly please contact us.
SADR - Sieve Analysis Dry < 212 micron: 99.5% < 150 micron: 99.2% < 106 micron: 98.0% < 63 micron: 97.9% < 45 micron: 96.
DS - Dry Strength (kgf/cm2) 35.0
WABS - Water absorption 1050C: 17% 1100C: 15% 1150C: 13% 1200C: 10% 1250C: 8%
FSHR - Firing Shrinkage 1100C: 0% 1150C: 1.5% 1200C: 3.0% 1250C: 5.0%

Out Bound Links

In Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="Clay 215" descrip="" searchkey="Kil 215" loi="8.90" casnumber="70694-09-6"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.200" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.600" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="1.900" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.200" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="0.600" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="25.000" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="59.500" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="2.200" tolerance=""/> </oxides> <volatiles> <volatile symbol="SO4" name="Sulfate" percent="0.570" tolerance=""/> <volatile symbol="Organics" name="" percent="0.360" tolerance=""/> <volatile symbol="C" name="Carbon" percent="0.210" tolerance=""/> <volatile symbol="LOI" name="Loss on Ignition" percent="8.900" tolerance=""/> </volatiles> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved