OxideAnalysisFormula
CaO0.10%0.005
MgO0.20%0.014
K2O2.40%0.070
Na2O0.10%0.004
TiO20.20%0.007
Al2O337.30%1.000
SiO247.00%2.139
Fe2O30.80%0.014
LOI12.00
Oxide Weight240.92
Formula Weight273.77
If this formula is not unified correctly please contact us.

Particle Size (e.s.d.)
125 microns - <0.03
10 microns - 96
2 microns - 51
1 microns - 35
Modulus of Rupture at 110C
Mn/M2 - 1.0
lbf/in2 - 140
Defloculant Required - (3:1 Na2SiO3(C.100):Na2CO3) - 0.0
Water Absorption
1120C - 20.5
1220C - 7.00
Shrinkage Dry to Fired
1120C - 9.50
1220C - 18.50
Reflectance 464nm
1120C - 86
1220C - 84
Refractoriness
Cone - 33, 1730C


Out Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="CC China Clay" descrip="Devon China Clay" searchkey="" loi="12.00" casnumber="70694-09-6"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.100" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.200" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="2.400" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.100" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="0.200" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="37.300" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="47.000" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="0.800" tolerance=""/> </oxides> <volatiles> <volatile symbol="LOI" name="Loss on Ignition" percent="12.000" tolerance=""/> </volatiles> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved