Allen G Kaolin

OxideAnalysisFormula
CaO0.05%0.002
MgO0.10%0.007
K2O0.20%0.006
Na2O0.08%0.003
TiO21.65%0.055
Al2O338.50%1.000
SiO245.00%1.984
Fe2O30.55%0.009
LOI13.60
Oxide Weight228.19
Formula Weight264.11
If this formula is not unified correctly please contact us.
SAMG - Surface Area (m2/gm) 13.5

An intermediate-grained kaolin used as a suspension aid in ceramic glazes.

Physical Properties
===================
Dry M.O.R., psi:* 400
pH: 4.8
C.E.C., meq/100g: 6.5 +/- 1.0
Specific Gravity: 2.6
P.C.E.: 33-34

Particle Size, Microns: 20 10 5 2 1 0.5 325# residue
(% finer than) 99% 97% 93% 81% 72% 56% .5

Fired Properties
================
Color, Cone 8 (L) 83.0
(a) -0.8
(b) 8.6

------------------
*Extruded, 50% ball clay, 50% flint
**50% Clay, 50% Nepheline Syenite


Out Bound Links


By Tony Hansen

XML for Import into INSIGHT

<?xml version="1.0" encoding="UTF-8"?> <material name="Allen G Kaolin" descrip="" searchkey="" loi="13.60" casnumber="95077-05-7"> <oxides> <oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.050" tolerance=""/> <oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.100" tolerance=""/> <oxide symbol="K2O" name="Potassium Oxide" status="" percent="0.200" tolerance=""/> <oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.080" tolerance=""/> <oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="1.650" tolerance=""/> <oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="38.500" tolerance=""/> <oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="45.000" tolerance=""/> <oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="0.550" tolerance=""/> </oxides> <volatiles> <volatile symbol="LOI" name="Loss on Ignition" percent="13.600" tolerance=""/> </volatiles> </material>


Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008, 2015 https://digitalfire.com, All Rights Reserved