BQ1000 - Plainsman Electric Bisque Firing Schedule
C04PLTP - Plainsman Typical Cone 04
C10RPL - Plainsman Cone 10R Firing
C6DHSC - Plainsman Cone 6 Slow Cool (Reactive glazes)
C6MSGL1 - Mastering Glazes Cone 6
C6PLST - Plainsman Cone 6 Electric Standard
FSCG1 - Shimbo Crystal Schedule 1
FSCGB1 - Bory 1 Fara Shimbo Crystalline Glaze
FSCGCL - Celestite
FSCGWM - Wollast-O-Matte Fara Shimbo Crystalline Glaze
FSCRGL - GC106 Base for Crystalline Glazes
FSHP1 - Shimbo Crystal Holding Pattern 1
FSHP2 - Shimbo Crystal Holding Pattern 2
FSHP3 - Shimbo Crystal Holding Pattern 3
FSNM5 - Fa's Number Five
PLC6CR - Cone 6 Crystal Glaze Plainsman
PLC6DS - Cone 6 Drop-and-Soak Firing Schedule
PLLFDS - Low Fire Drop-and-Hold

FSCGWM Firing Schedule

Wollast-O-Matte Fara Shimbo Crystalline Glaze

Step °C °F Hold Time
1 100°C/hr to 200C  180°F/hr to 392F  0 2:02  
2 250°C/hr to 500C  450°F/hr to 932F  0 3:14  
3 500°C/hr to 1275C  900°F/hr to 2327F  0 4:47  
4 9999°C/hr to 1150C  17998°F/hr to 2102F  0 4:48  
5 30°C/hr to 1080C  54°F/hr to 1976F  0 7:08  
Start temperature assumed: 25°C or 75°F

Links

Typecodes Oxidation Firing

By Tony Hansen


Tell Us How to Improve This Page

We are experiencing issues with this messaging system.
These are related to network and server improvements being made.
We are working on it now, please check back again later.

Or ask a question and we will alter this page to better answer it.

Email Address

Name

Subject

Message


Upload picture


Copyright 2008, 2015, 2017 https://digitalfire.com, All Rights Reserved