Ravenscrag Recipe H: Oatmeal Matte| Code | GR6-H |
| Modification Date | 2011-01-31 15:26:30 |
| Member of Group | RV6 |
| Description | Plainsman Cone 6 Ravenscrag Slip Glaze |
Recipe| Material | Amount | Units | +/- | *Stat |
| Ravenscrag Slip | 60.00 | kg | | |
| Calcined Alumina | 10.00 | kg | | |
| Dolomite | 10.00 | kg | | |
| Ferro Frit 3134 | 20.00 | kg | | |
| Manganese Dioxide | 4.00 | kg | | |
| Rutile | 5.00 | kg | | |
| Illmenite Granular | 0.30 | kg | | |
| | 109.30 | |
Firing Schedule
| Rate (C) | Temp (C) | Hold (Min) | Step | | 55 | 104 | 120 | 1 | | 167 | 482 | 0 | 2 | | 83 | 593 | 0 | 3 | | 167 | 945 | 0 | 4 | | 60 | 1185 | 20 | 5 | | 278 | 1035 | 0 | 6 | | 83 | 816 | 0 | 7 |
|